17-4PH | ||||
Chemical composition: C=0.7%max, Mn=1%max, Cr=17%, Ni=4%, Cu=4%, Cb+Ta=0.3% | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 7.75 *10³ | kg/m³ | 484 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 196 | GPa | 28400 | ksi |
Thermal expansion (20 ºC) | 10.8*10-6 | ºCˉ¹ | 6.0*10-6 | in/(in* ºF) |
Specific heat capacity | 460 | J/(kg*K) | 0.11 | BTU/(lb*ºF) |
Thermal conductivity | 18.4 | W/(m*K) | 128 | BTU*in/(hr*ft²*ºF) |
Electric resistivity | 8*10-7 | Ohm*m | 8*10-5 | Ohm*cm |
Tensile strength (annealed) | 1030 | MPa | 150000 | psi |
Yield strength (annealed) | 760 | MPa | 110000 | psi |
Elongation (annealed) | 10 | % | 10 | % |
Hardness (annealed) | 33 | RC | 33 | RC |
Tensile strength (cold drawn) | 1380 | MPa | 200000 | psi |
Yield strength (cold drawn) | 1230 | MPa | 178000 | psi |
Elongation (cold drawn) | 12 | % | 12 | % |
Hardness (cold drawn) | 44 | RC | 44 | RC |