AISI 304 | ||||
Chemical composition: C=0.08%max, Mn=2%max, Cr=19%, Ni=9.5% | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 7.9 *10³ | kg/m³ | 493 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 193 | GPa | 28000 | ksi |
Thermal expansion (20 ºC) | 17.2*10-6 | ºCˉ¹ | 9.5*10-6 | in/(in* ºF) |
Specific heat capacity | 502 | J/(kg*K) | 0.12 | BTU/(lb*ºF) |
Thermal conductivity | 16.2 | W/(m*K) | 112 | BTU*in/(hr*ft²*ºF) |
Electric resistivity | 7.2*10-7 | Ohm*m | 7.2*10-5 | Ohm*cm |
Tensile strength (annealed) | 586 | MPa | 85000 | psi |
Yield strength (annealed) | 241 | MPa | 35000 | psi |
Elongation (annealed) | 55 | % | 55 | % |
Hardness (annealed) | 80 | RB | 80 | RB |
Tensile strength (1/2 hard) | 1100 | MPa | 160000 | psi |
Yield strength (1/2 hard) | 760 | MPa | 110000 | psi |
Elongation (1/2 hard) | 10 | % | 10 | % |
Hardness (1/2 hard) | 35 | RC | 35 | RC |