SAE 4340 | ||||
Chemical composition: C=0.40%, Mn=0.7%, Mo=0.25%, Cr=0.8%, Ni-1.8% | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 7.872 *10³ | kg/m³ | 491.4 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 205 | GPa | 29700 | ksi |
Thermal expansion (20 ºC) | 12.6*10-6 | ºCˉ¹ | 7.00*10-6 | in/(in* ºF) |
Specific heat capacity | 477 | J/(kg*K) | 0.114 | BTU/(lb*ºF) |
Thermal conductivity | 44.6 | W/(m*K) | 309 | BTU*in/(hr*ft²*ºF) |
Electric resistivity | 2.48*10-7 | Ohm*m | 2.48*10-5 | Ohm*cm |
Tensile strength (annealed) | 745 | MPa | 108000 | psi |
Yield strength (annealed) | 472 | MPa | 68500 | psi |
Elongation (annealed) | 28 | % | 22 | % |
Hardness (annealed) | 96 | RB | 96 | RB |
Tensile strength (normalized) | 1279 | MPa | 195500 | psi |
Yield strength (normalized) | 862 | MPa | 125000 | psi |
Elongation (normalized) | 20 | % | 12 | % |
Hardness (normalized) | 40 (112) | RC (RB) | 40 (112) | RC (RB) |