Wrought magnesium alloy ZK60A | ||||
Chemical composition: Zn=5.5%, Zr=0.45% min., Mg balance | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 1.83 *10³ | kg/m³ | 114 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 45 | GPa | 6530 | ksi |
Thermal expansion (20 ºC) | 26.0*10-6 | ºCˉ¹ | 14.4*10-6 | in/(in* ºF) |
Specific heat capacity | 1000 | J/(kg*K) | 0.239 | BTU/(lb*ºF) |
Thermal conductivity | 120 | W/(m*K) | 833 | BTU*in/(hr*ft²*ºF) |
Electric resistivity | 6.0*10-8 | Ohm*m | 6.0*10-6 | Ohm*cm |
Tensile strength (F) | 340 | MPa | 49300 | psi |
Yield strength (F) | 260 | MPa | 37700 | psi |
Elongation (F) | 11 | % | 11 | % |
Shear strength (F) | 185 | MPa | 26800 | psi |
Hardness (F) | 75 | HB(500) | 75 | HB(500) |
Tensile strength (T5) | 365 | MPa | 52900 | psi |
Yield strength (T5) | 305 | MPa | 44200 | psi |
Elongation (T5) | 11 | % | 11 | % |
Shear strength (T5) | 180 | MPa | 26100 | psi |
Hardness (T5) | 88 | HB(500) | 88 | HB(500) |
Annealing temperature | 290 | ºC | 554 | ºF |
Liquidus temperature | 635 | ºC | 1175 | ºF |
Solidus temperature | 520 | ºC | 968 | ºF |