Titanium alpha alloy, Grade 6 (Ti-5Al-2.5Sn)

(submitted by the website administration)

Titanium α-alloy, Grade 6 (Ti-5Al-2.5Sn)
Chemical composition: O=0.2% max., Fe=0.5% max., Al=5%, Sn=2.5%, Ti balance
Property Value in metric unit Value in US unit
Density 4.48 *10³ kg/m³ 280 lb/ft³
Modulus of elasticity 117 GPa 17000 ksi
Thermal expansion (20 ºC) 9.4*10-6 ºCˉ¹ 5.2*10-6 in/(in* ºF)
Specific heat capacity 530 J/(kg*K) 0.127 BTU/(lb*ºF)
Thermal conductivity 7.8 W/(m*K) 54 BTU*in/(hr*ft²*ºF)
Electric resistivity 160*10-8 Ohm*m 160*10-6 Ohm*cm
Tensile strength 862 MPa 125000 psi
Yield strength 807 MPa 117000 psi
Elongation 16 % 16 %
Hardness 34 HRC 34 HRC
Melting temperature 1600 ºC 2910 ºF
Beta Transus temperature 1038 ºC 1900 ºF