USA: AISI S1, UK: BS1, Sweden: 2710, Germany: 1.2542, Japan: SKS41 | ||||
Chemical composition: C=0.5%, Mn=0.3%, W=2.5%, Si=0.3%, Cr=1.5% | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 7.8 *10³ | kg/m³ | 486.9 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 207 | GPa | 30000 | ksi |
Thermal expansion (20 ºC) | 10.9*10-6 | ºCˉ¹ | 6.0*10-6 | in/(in* ºF) |
Specific heat capacity | 461 | J/(kg*K) | 0.11 | BTU/(lb*ºF) |
Thermal conductivity | 31.9 | W/(m*K) | 221 | BTU*in/(hr*ft²*ºF) |
Annealing temperature | 740...760 | ºC | 1365...1400 | ºF |
Quenching temperature | 860...900 | ºC | 1580...1650 | ºF |
Tempering temperature | 175...480 | ºC | 350...900 | ºF |
Hardness (annealed) | 98 | RB | 98 | RB |
Hardness (hardened) | 62 | RC | 62 | RC |
Quenching medium | Oil | |||
Hardening depth | Medium | |||
Resistivity to distortion | Medium | |||
Resistivity to cracking | High | |||
Machinability | Medium | |||
Toughness | High | |||
Wear resistance | Medium |