Main page
About us
Sliding Bearings Consulting
Advertising Opportunities
to Wrought brasses
to Properties of copper alloys
(submitted by the website administration)
Wrought copper alloy C46400 (Uninhibited Naval Brass) | ||||
Chemical composition: Zn=39.2%, Sn=0.7%, Cu=60% | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 8.41 *10³ | kg/m³ | 525 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 103 | GPa | 15000 | ksi |
Thermal expansion (20 ºC) | 21.2*10-6 | ºCˉ¹ | 11.8*10-6 | in/(in* ºF) |
Specific heat capacity | 377 | J/(kg*K) | 0.090 | BTU/(lb*ºF) |
Thermal conductivity | 116 | W/(m*K) | 804 | BTU*in/(hr*ft²*ºF) |
Electric resistivity | 6.63*10-8 | Ohm*m | 6.63*10-6 | Ohm*cm |
Tensile strength (annealed) | 400 | MPa | 58000 | psi |
Yield strength (annealed) | 172 | MPa | 25000 | psi |
Elongation (annealed) | 49 | % | 49 | % |
Shear strength (annealed) | 276 | MPa | 40000 | psi |
Hardness (annealed) | 55 | R30T | 55 | R30T |
Tensile strength (cold work) | 483 | MPa | 70000 | psi |
Yield strength (cold work) | 400 | MPa | 58000 | psi |
Elongation (cold work) | 17 | % | 17 | % |
Shear strength (cold work) | 296 | MPa | 43000 | psi |
Hardness (cold work) | 68 | R30T | 68 | R30T |
Annealing temperature | 425-600 | ºC | 800-1100 | ºF |
Liquidus temperature | 899 | ºC | 1650 | ºF |
Solidus temperature | 888 | ºC | 1630 | ºF |