Wrought copper alloy C63000 (Aluminum Bronze) | ||||
Chemical composition: Al=10.0%, Fe=3.0%, Ni=5%, Cu=balance | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 7.58 *10³ | kg/m³ | 473 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 121 | GPa | 17500 | ksi |
Thermal expansion (20 ºC) | 16.2*10-6 | ºCˉ¹ | 9.0*10-6 | in/(in* ºF) |
Specific heat capacity | 377 | J/(kg*K) | 0.090 | BTU/(lb*ºF) |
Thermal conductivity | 39.1 | W/(m*K) | 271 | BTU*in/(hr*ft²*ºF) |
Electric resistivity | 19.3*10-8 | Ohm*m | 19.3*10-6 | Ohm*cm |
Tensile strength (as fabricat.) | 689 | MPa | 100000 | psi |
Yield strength (as fabricated) | 414 | MPa | 60000 | psi |
Elongation (as fabricated) | 15 | % | 15 | % |
Shear strength (as fabricated) | 427 | MPa | 62000 | psi |
Fatigue strength (as fabricat.) | 248 | MPa | 36000 | psi |
Hardness (as fabricated) | 96 | RB | 96 | RB |
Tensile strength (cold.work+ann.) | 814 | MPa | 118000 | psi |
Yield strength (cold work+ann.) | 517 | MPa | 75000 | psi |
Elongation (cold work+anneal) | 15 | % | 15 | % |
Shear strength (cold work+ann.) | 483 | MPa | 70000 | psi |
Fatigue strength (cold work+ann.) | 255 | MPa | 37000 | psi |
Hardness (cold work+anneal) | 98 | RB | 98 | RB |
Annealing temperature | 650-815 | ºC | 1200-1500 | ºF |
Liquidus temperature | 1054 | ºC | 1930 | ºF |
Solidus temperature | 1035 | ºC | 1895 | ºF |