Wrought copper alloy C36000 (Free-Cutting Brass)
Chemical composition: Zn=35.4%, Pb=3.1%, Cu=61.5%
Property Value in metric unit Value in US unit
Density 8.50 *10³ kg/m³ 531 lb/ft³
Modulus of elasticity 96.5 GPa 14000 ksi
Thermal expansion (20 ºC) 20.5*10-6 ºCˉ¹ 11.4*10-6 in/(in* ºF)
Specific heat capacity 377 J/(kg*K) 0.090 BTU/(lb*ºF)
Thermal conductivity 116 W/(m*K) 804 BTU*in/(hr*ft²*ºF)
Electric resistivity 6.63*10-8 Ohm*m 6.63*10-6 Ohm*cm
Tensile strength (as fabricat.) 338 MPa 49000 psi
Yield strength (as fabricated) 124 MPa 18000 psi
Elongation (as fabricated) 50 % 50 %
Shear strength (as fabricated) 207 MPa 30000 psi
Hardness (as fabricated) 68 RF 68 RF
Tensile strength (cold work) 386 MPa 56000 psi
Yield strength (cold work) 310 MPa 45000 psi
Elongation (cold work) 20 % 20 %
Shear strength (cold work) 228 MPa 33000 psi
Hardness (cold work) 62 RB 62 RB
Annealing temperature 425-600 ºC 800-1100 ºF
Liquidus temperature 899 ºC 1650 ºF
Solidus temperature 888 ºC 1630 ºF