Cast copper alloy C87500 (Silicon Bronze/Silicon Brass) | ||||
Chemical composition: Zn=14%, Si=4.0%, Cu=82% | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 8.28 *10³ | kg/m³ | 517 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 106 | GPa | 15400 | ksi |
Thermal expansion (20 ºC) | 19.6*10-6 | ºCˉ¹ | 10.9*10-6 | in/(in* ºF) |
Specific heat capacity | 377 | J/(kg*K) | 0.090 | BTU/(lb*ºF) |
Thermal conductivity | 27.7 | W/(m*K) | 192 | BTU*in/(hr*ft²*ºF) |
Electric resistivity | 25.6*10-8 | Ohm*m | 25.6*10-6 | Ohm*cm |
Tensile strength (sand cast) | 462 | MPa | 67000 | psi |
Yield strength (sand cast) | 207 | MPa | 30000 | psi |
Elongation (sand cast) | 21 | % | 21 | % |
Fatigue strength (sand cast) | 152 | MPa | 22000 | psi |
Hardness (sand cast) | 134 | HB(3000) | 134 | HB(3000) |
Liquidus temperature | 916 | ºC | 1680 | ºF |
Solidus temperature | 821 | ºC | 1510 | ºF |