According to the Unified Numbering System (UNS):

Cast Silicon Bronzes (Silicon Brasses) are copper alloys, containing 3.0-4.5% of silicon (Si) and up to 20% of zinc (Zn) as major alloying elements. Cast Silicon Bronzes are designated with the numbers from C87000 through C87999.

Cast Silicon Bronzes may contain manganese (Mn) and phosphorous (P) as additional alloying elements.

Silicon Bronzes have mono-phase structure (α-phase).

Cast Silicon Bronzes have moderate mechanical strength combined with very good aqueous and atmospheric corrosion resistance and very good weldability.

Cast Silicon Bronzes are used for manufacturing decorative items, bearings, window hardware, gears, impellers, pump and valve components, plumbing fittings.

Chemical compositions of some cast silicon bronzes (silicon brasses)

UNS Designation Zn,% Si,% Mn,% P,% Cu,%
C87300 0.25 max. 3.5-4.5 0.8-1.5 - balance
C87400 12.0-16.0 2.5-4.0 - - balance
C87500 12.0-16.0 3.0-5.0 - - balance
C87600 4.0-7.0 3.5-5.5 - - balance
C87850 balance 2.7-3.4 - 0.05-0.20 balance

Properties of some cast silicon bronzes and silicon brasses

Related internal links

cast_silicon_bronzes_and_silicon_brasses.txt · Last modified: 2023/12/13 by dmitri_kopeliovich
Promote in SubsTech       Creative Commons License Except where otherwise noted, this work is licensed under a Creative Commons Attribution-Noncommercial-Share Alike 3.0 License