to Silver alloys
to Properties of silver alloys
(submitted by the website administration)
Silver-ABA | ||||
Chemical composition: Ag=92.75%, Cu=5.0%, Ti=1.25%, Al-1.0% | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 10.0 *10³ | kg/m³ | 5.27 | Troy oz/in³ |
---|---|---|---|---|
Modulus of elasticity | 77 | GPa | 11170 | ksi |
Thermal expansion (20 ºC) | 2.07*10-5 | ºCˉ¹ | 1.15*10-5 | in/(in* ºF) |
Thermal conductivity | 344 | W/(m*K) | 2385 | BTU*in/(hr*ft²*ºF) |
Electrical resistivity | 2.2*10-8 | Ohm*m | 2.2*10-6 | Ohm*cm |
Tensile strength | 136 | MPa | 20000 | psi |
Yield strength | 282 | MPa | 41000 | psi |
Elongation | 37 | % | 37 | % |