Fine silver
Chemical composition: Ag=99.90% min.
Property Value in metric unit Value in US unit
Density 10.49 *10³ kg/m³ 5.527 Troy oz/in³
Modulus of elasticity 83 GPa 12000 ksi
Thermal expansion (20 ºC) 1.9*10-5 ºCˉ¹ 1.06*10-5 in/(in* ºF)
Specific heat capacity 235 J/(kg*K) 0.0561 BTU/(lb*ºF)
Thermal conductivity 429 W/(m*K) 2974 BTU*in/(hr*ft²*ºF)
Electrical resistivity 1.642*10-8 Ohm*m 1.642*10-6 Ohm*cm
Tensile strength (annealed) 125 MPa 18000 psi
Yield strength (annealed) 54 MPa 7800 psi
Elongation (annealed) 25 min. % 25 min. %
Tensile strength (1/2 hard) 235 MPa 34000 psi
Elongation (1/2 hard) 8 % 8 %
Tensile strength (full hard) 275 MPa 40000 psi
Elongation (full hard) 3 % 3 %
Tensile strength (spring hard) 330 MPa 48000 psi
Elongation (spring hard) 1 % 1 %
Melting point 960.8 ºC 1761 ºF
Boiling point 2210 ºC 4010 ºF