USA: AISI A2, UK: BA2, Sweden: 2260, Germany: 1.2363, Japan: SKD12 | ||||
Chemical composition: C=1%, Mn=0.3%, Si=0.3%, Cr=5%, Mo=1% | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 7.81 *10³ | kg/m³ | 487.8 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 190 | GPa | 27500 | ksi |
Thermal expansion (20 ºC) | 10.6*10-6 | ºCˉ¹ | 5.9*10-6 | in/(in* ºF) |
Specific heat capacity | 461 | J/(kg*K) | 0.11 | BTU/(lb*ºF) |
Thermal conductivity | 26 | W/(m*K) | 180 | BTU*in/(hr*ft²*ºF) |
Annealing temperature | 840...870 | ºC | 1545...1600 | ºF |
Quenching temperature | 950...980 | ºC | 1740...1800 | ºF |
Tempering temperature | 175...480 | ºC | 350...900 | ºF |
Hardness (annealed) | 97 | RB | 97 | RB |
Hardness (hardened) | 65 | RC | 65 | RC |
Quenching medium | Air | |||
Hardening depth | High | |||
Resistivity to distortion | Very high | |||
Resistivity to cracking | Very high | |||
Machinability | Medium | |||
Toughness | Medium | |||
Wear resistance | High |